C46750

Naval Brass C46750 is a copper-zinc-tin alloy designed for excellent corrosion resistance in marine environments, with good strength, hardness, and wear resistance. It is widely used in shipbuilding, marine hardware, and industrial applications requiring durability against seawater.

Chemical Composition

Elements Min (%) Max (%)
Cu 59.20 62.50
Sn 1.00 1.80
Pb 0.00 0.25
Zn Remainder
Fe 0.00 0.10
Ni 0.00 0.50
Sb 0.05 0.15
P 0.05 0.15

Mechanical properties according to ASTM B21 C46750 (As per temper H50)

Range (inch) UTS Min
(ksi)
UTS Max
(ksi)
PS Min
(ksi)
Elongation Min
(%)
Hardness
Hardness Min
(HRB)
Hardness Max
(HRB)
Round (Dia) 0.300 – 0.500 48 20 5
0.500 – 1.000 48 20 10
1.000 – 2.000 48 20 15
Hex (A/F) 0.300 – 0.500 48 20 5
0.500 – 1.000 48 20 10
1.000 – 2.000 48 20 15
Square (A/F) 0.300 – 0.500 48 20 5
0.500 – 1.000 48 20 10
1.000 – 2.000 48 20 15
Rectangle Thickness: 0.300 – 0.500 48 20 5
Width: 0.500 – 1.000
Thickness: 0.500 – 1.000 48 20 10
Width: 1.000 – 2.000
Thickness: 1.000 – 2.000 48 20 15
Width: 2.000 – 3.000
Range (mm) UTS Min
(MPa)
UTS Max
(MPa)
PS Min
(MPa)
Elongation Min
(%)
Hardness Min
(HRB)
Hardness Max
(HRB)
Round (Dia) 8 12 315 140 5
13 25 315 140 10
25 50 315 140 15
Hex (A/F) 8 12 315 140 5
13 25 315 140 10
25 50 315 140 15
Square (A/F) 8 12 315 140 5
13 25 315 140 10
25 50 315 140 15
Rectangle Thickness 8 – 12 315 140 5
Width 12 – 25
Thickness 13 – 25 315 140 10
Width 25 – 50
Thickness 25 – 50 315 140 15
Width 50 – 75

PHYSICAL PROPERTIES
Melting Range 1546–1632 °F
Density 0.31 lb/cu in (8.48 g/cm³)
Electrical Conductivity ~22% IACS
Thermal Conductivity 59.6 Btu/sq. ft/ft hr/°F
Coefficient of Thermal Expansion 10 × 10⁻⁶ per °F (68–212°F)
FABRICATION PROPERTIES
Technique Suitability
Hot Working Excellent
Cold Working Moderate
Machinability Good
Soldering and brazing Good
Welding Fair

Typical Uses